摘要
Bi 2 Sr 2 Co 2 O y with excellent thermoelectric properties has received extensive attention from scientific researchers. In this study, Bi 2 Sr 2 Co 2 O y ceramic samples were prepared using the solid-phase sintering method. By Ag + substitution for Bi 3+ , the hole concentration and electrical conductivity were optimised. On this basis, nano-SiC particles were introduced to increase grain boundaries, improve phonon scattering, reduce the mean free path of phonons, and reduce the lattice thermal conductivity . A sample with a nominal composition of Bi 1.8 Ag 0.2 Sr 2 Co 2 O y + 0.025 wt% SiC had a maximum ZT value of 0.35 at 923 K, which was approximately 67 % higher than the ZT value of pure Bi 2 Sr 2 Co 2 O y . These results confirmed that under the combined action of Ag substitution and SiC doping, the thermoelectric performance of Bi 2 Sr 2 Co 2 O y was significantly improved.