This work proposes the roasting of amblygonite with calcium sulfate followed by water leaching to extract lithium and phosphorus. Various roasting parameters including roasting temperature, the mass ratio CaSO 4 /ore, roasting time as well as leaching parameters, such as the liquid/solid ratio, temperature and time, have been carefully investigated. The lithium extraction efficiency can be as high as 99.8% with a mass ratio of CaSO 4 /ore of 0.85 after roasting at 775 °C for 1 h and water leaching at a liquid/solid ratio of 3 mL/g at 100 °C for 2 h. The XRD analysis demonstrates that the fluoride in the amblygonite can be converted into Ca 5 (PO 4 ) 3 F and CaF 2 . Lithium in the leach liquor can be recovered as Li 2 CO 3 . Meanwhile, the phosphorus in the water leach residue can be recovered as FePO 4 with a high recovery of 96.6% after acid dissolution and precipitation, which can be further treated to produce LiFePO 4 .