In this paper, the effects of the matrix pore structure on the strength and corrosion resistance of corundum castables are reported. Pore diameters of castables fired at 110 °C could be decreased from 550 nm to 72 nm when 4% Al 2 O 3 -SiO 2 gel powder was added. The pore diameter of the castables decreased from 850 nm to 500 nm after firing at 1100 °C, but increased from approximately 2 μm–8 μm after firing at 1500 °C. The strength of castables fired at 1500 °C increased remarkably with the addition of Al 2 O 3 -SiO 2 gel powder. A maximum cold modulus of rupture (CMOR) of 62.34 MPa was obtained when 4% Al 2 O 3 -SiO 2 gel powder was added. After slag corrosion, the penetration index fell from 16.6% to 4%, suggesting that a homogeneous pore size distribution and a smaller pore size played an important role in improving the penetration resistance.